- Cold rolled strips: 0.03~0.l0×180~250mm >0.10~1.00×10~250mm >1.00~2.50×100~250mm 2. Cold drown wires: 0.l0~6.00mm 3. Hot rolled flat products: 4.50~20.0×50~250mm 4. Hot forged bars: Φ20.0~100.0mm / bar
Grade | U.K. | Germany | U.S.A. | Russia | Standard |
1J22 | Permendur | Vacoflux 50 | Supermendur HiperCo50 | 50КФ | GB/T15002-1994 |
Grade | Chemical Composition (%) | |||||||||
C≤ | Mn≤ | Si≤ | P≤ | S≤ | Cu≤ | Ni≤ | Co | V | Fe | |
1J22 | 0.04 | 0.30 | 0.30 | 0.020 | 0.020 | 0.20 | 0.50 | 49.0~51.0 | 0.80~1.80 | Balance |
Grade | Resistivity /(μΩ•m) | Density/(g/cm3) | Curie point/°C | Magnetostriction Cofficient/(×10-6) | Tensile Strength,N/mm2 | |
Unannealed | Annealed | |||||
1J22 | 0.40 | 8.20 | 980 | 60~100 | 1325 | 490 |
Thermal Expansion Coefficient (20~100ºC) | 8.5*10-6/ºC |
Volume Resistivity (20ºC) | 40 μΩ.cm |
Coercive Force | 128 A/m |
Magnetic induction strength in different magnetic field | |
B400 | 1.6 |
B800 | 1.8 |
B1600 | 2.0 |
B2400 | 2.1 |
B4000 | 2.15 |
B8000 | 2.2 |